Soft Ground with Water-Soluble Ink and Acrylic Mediums Test 13

Test Summary
I am testing a soft ground mixture that consists of 3 parts Graphic Chemical Water based Block Printing Ink Peacock Blue, 2 parts Golden Acrylic Silkscreen Medium, and 1/2 part Golden GAC 200. In am using newsprint as the transfer paper. The ink was refrigerated in hopes of extending the drawing time of the ground.

Date: February 6, 2009
Researcher’s Name: Esther White
Plate Material: .032 Copper
Plate Size: 4 in x 3 in
Room Temperature: 77° F

Plate Preparation
I degreased the plate with Bon-Ami and water made into a paste. The paste was rubbed across the plate surface and rinsed away with water. The copper plate was blow dried and finished with a clean towel. I rolled a thin amount of ground across the plate’s surface just enough so that you could not see the copper sparkle through the ground. I waited 10 minutes before placing the newsprint onto the grounded copper plate. I drew for 40 minutes near an open window before the ground became too difficult to draw through. The surface of the plate became smudgy and predictably more difficult to work as time progressed.

Esther's Drawing and Transfer

Esther’s Drawing and Transfer

Etching Notes
The plate was etched in a vertical etching tank filled with 35° Baume Ferric Chloride.

Timed Application of Mordant
50 Minutes

Esther's Etched Plate

Esther’s Etched Plate

Inking Methods
The plate was inked with unmodified 50% Graphic Chemical Bone Black and 50% Graphic Chemical Stiff Black. The ink was carded on with a orange plastic scraper, wiped with used tarlatan, and hand wiped.

Paper Type: Hahnemule Copperplate
Paper Soaking Time: 20 Minutes
Press Blanket Setup: Small Takach, 2 Blankets, 8.0 pressure

Test Conclusion
The print failed because of a mistake drying the ground on the copper plate.

Printed Images

Esther's Printed Proof

Esther’s Printed Proof

Soft Ground with Water-Soluble Ink and Acrylic Mediums Test 14 >